# Al–Mo system

> Al–Mo system: 203 accepted literature values (invariant reaction 94, crystal structure 36, phase equilibrium 29, formation 29) and 6 calculated phase diagram(s) from ORCHID, each value with evidence class, source, page and quote.

HTML: https://data.orchid-project.org/systems/AL-MO.html · Markdown: https://data.orchid-project.org/systems/AL-MO.md

203 accepted literature values from 5 paper(s) (experimental 76, model 62, unspecified 65); 6 calculated phase diagram(s). 35 further extracted value(s) not accepted by the reader-agreement checks are only in the JSON/CSV.

Data: [JSON](https://data.orchid-project.org/literature/systems/AL-MO.json) · [CSV](https://data.orchid-project.org/systems/AL-MO.csv) · [interactive explorer](https://orchid-project.org/data-explorer/#AL-MO) · [interactive phase diagram](https://orchid-project.org/phase-diagrams/#AL-MO/AlMo-09Du.json) · [phases (15)](https://data.orchid-project.org/phases/pages/AL-MO.html) · [papers (bibliography)](https://data.orchid-project.org/bibliography/pages/systems/AL-MO.html) · [Markdown](https://data.orchid-project.org/systems/AL-MO.md)

Table: Accepted values by evidence class

| Evidence class | Values |
|---|---:|
| experimental | 76 |
| model | 62 |
| unspecified | 65 |

Table: Accepted values by property group

| Property group | Values |
|---|---:|
| invariant reaction | 94 |
| phase transition | 7 |
| phase equilibrium | 29 |
| formation | 29 |
| mixing / partial | 8 |
| crystal structure | 36 |

## Calculated phase diagrams

Binary phase diagrams calculated with pycalphad 0.11.2 from the SGTE binary collection (Hallstedt 2025, CC BY 4.0). Evidence class: model.

Table: Assessments with a calculated phase diagram

| TDB file | Assessment | SHA-256 | Links |
|---|---|---|---|
| AlMo-09Du.tdb | Z. Du, C. Guo, C. Li, W. Zhang, J. Phase Equilib. Diffus., 30, 487-501(2009). [doi:10.1007/s11669-009-9564-4](https://doi.org/10.1007/s11669-009-9564-4) | `2eb56c9f752986706a80dc69aa802fd653c181022670f3357b6fe63dd2b50a9c` | [viewer](https://orchid-project.org/phase-diagrams/#AL-MO/AlMo-09Du.json) · [TDB](https://orchid-project.org/data/databases/sgte-binary/AlMo-09Du.tdb) · [JSON](https://data.orchid-project.org/phase-diagrams/sgte/AlMo-09Du.json) |
| AlMo-10Cup.tdb | D.M. Cupid, O. Fabrichnaya, F. Ebrahimi, H.J. Seifert, Intermetallics, 18, 1185-96(2010). [doi:10.1016/j.intermet.2010.03.010](https://doi.org/10.1016/j.intermet.2010.03.010) | `87c3f97cf72fd3363cd0bfedde18f2af85dd5dc85fa517e033c4b0666b427230` | [viewer](https://orchid-project.org/phase-diagrams/#AL-MO/AlMo-10Cup.json) · [TDB](https://orchid-project.org/data/databases/sgte-binary/AlMo-10Cup.tdb) · [JSON](https://data.orchid-project.org/phase-diagrams/sgte/AlMo-10Cup.json) |
| AlMo-16Pen.tdb | J. Peng, P. Franke, D. Manara, T. Watkins, R.J.M. Konings, H.J. Seifert, J. Alloys Compd., 674, 305-14(2016). [doi:10.1016/j.jallcom.2016.03.044](https://doi.org/10.1016/j.jallcom.2016.03.044) | `b64c311d043cc74d1a6a0e7c20632dd1638ed15c41034a3adce1b72852ec6e64` | [viewer](https://orchid-project.org/phase-diagrams/#AL-MO/AlMo-16Pen.json) · [TDB](https://orchid-project.org/data/databases/sgte-binary/AlMo-16Pen.tdb) · [JSON](https://data.orchid-project.org/phase-diagrams/sgte/AlMo-16Pen.json) |
| AlMo-97Cos.tdb | A. Costa e Silva, M.J. Kaufman, Z. Metallkd., 88, 854-65(1997). [doi:10.3139/ijmr-1997-0159](https://doi.org/10.3139/ijmr-1997-0159) | `ddd7a660ca5292b2388b01219b5f59d8606813bd40130d06c949607d61e9e94c` | [viewer](https://orchid-project.org/phase-diagrams/#AL-MO/AlMo-97Cos.json) · [TDB](https://orchid-project.org/data/databases/sgte-binary/AlMo-97Cos.tdb) · [JSON](https://data.orchid-project.org/phase-diagrams/sgte/AlMo-97Cos.json) |
| AlMo-97Sau.tdb | N. Saunders, J. Phase Equilib., 18, 370-78(1997). [doi:10.1007/s11669-997-0063-1](https://doi.org/10.1007/s11669-997-0063-1) | `709eda501ac1bee8a78580b75d94905a84605709c44753a77a7f459132c943dc` | [viewer](https://orchid-project.org/phase-diagrams/#AL-MO/AlMo-97Sau.json) · [TDB](https://orchid-project.org/data/databases/sgte-binary/AlMo-97Sau.tdb) · [JSON](https://data.orchid-project.org/phase-diagrams/sgte/AlMo-97Sau.json) |
| AlMo-98Sau-LB.tdb | N. Saunders, COST 507, Final report round 2, 1998. | `bc4d36f89701a2a519b181f9809ed3316ba79eff876a5e5a796f48dc3ad4da7f` | [viewer](https://orchid-project.org/phase-diagrams/#AL-MO/AlMo-98Sau-LB.json) · [TDB](https://orchid-project.org/data/databases/sgte-binary/AlMo-98Sau-LB.tdb) · [JSON](https://data.orchid-project.org/phase-diagrams/sgte/AlMo-98Sau-LB.json) |

Table: Calculated three-phase invariants (model, mole fraction of the second component)

| TDB file | T (K) | Phases at the invariant |
|---|---:|---|
| AlMo-09Du.tdb | 2422.65 | LIQUID (x(Mo) 0.71551) + ALMO3_A15 (x(Mo) 0.75202) + BCC_A2 (x(Mo) 0.77666) |
| AlMo-09Du.tdb | 1993.05 | LIQUID (x(Mo) 0.43783) + BCC_A2 (x(Mo) 0.55233) + ALMO3_A15 (x(Mo) 0.73154) |
| AlMo-09Du.tdb | 1843.18 | LIQUID (x(Mo) 0.35454) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.47815) |
| AlMo-09Du.tdb | 1843.18 | LIQUID (x(Mo) 0.35462) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.47823) |
| AlMo-09Du.tdb | 1814.37 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.30828) + AL63MO37 (x(Mo) 0.37) |
| AlMo-09Du.tdb | 1814.37 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.3087) + AL63MO37 (x(Mo) 0.37) |
| AlMo-09Du.tdb | 1814.37 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.30811) + AL63MO37 (x(Mo) 0.37) |
| AlMo-09Du.tdb | 1763.03 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.48168) |
| AlMo-09Du.tdb | 1763.03 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.48177) |
| AlMo-09Du.tdb | 1763.03 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.48176) |
| AlMo-09Du.tdb | 1743.01 | AL8MO3 (x(Mo) 0.27273) + BCC_A2 (x(Mo) 0.49135) + ALMO3_A15 (x(Mo) 0.73313) |
| AlMo-09Du.tdb | 1495.13 | LIQUID (x(Mo) 0.06265) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-09Du.tdb | 1495.13 | LIQUID (x(Mo) 0.06269) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-09Du.tdb | 1424.97 | LIQUID (x(Mo) 0.04818) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-09Du.tdb | 1424.97 | LIQUID (x(Mo) 0.04821) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-09Du.tdb | 1424.97 | LIQUID (x(Mo) 0.04826) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-09Du.tdb | 1266.63 | LIQUID (x(Mo) 0.02268) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-09Du.tdb | 1266.63 | LIQUID (x(Mo) 0.02271) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-09Du.tdb | 1266.63 | LIQUID (x(Mo) 0.02265) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-09Du.tdb | 1218.43 | LIQUID (x(Mo) 0.01685) + AL22MO5 (x(Mo) 0.18519) + AL17MO4 (x(Mo) 0.19048) |
| AlMo-09Du.tdb | 1218.43 | LIQUID (x(Mo) 0.0168) + AL22MO5 (x(Mo) 0.18519) + AL17MO4 (x(Mo) 0.19048) |
| AlMo-09Du.tdb | 1215 | AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-09Du.tdb | 1118.96 | LIQUID (x(Mo) 0.00793) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-09Du.tdb | 1118.96 | LIQUID (x(Mo) 0.00793) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-09Du.tdb | 1118.96 | LIQUID (x(Mo) 0.00792) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-09Du.tdb | 1017.49 | AL17MO4 (x(Mo) 0.19048) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-09Du.tdb | 984.95 | LIQUID (x(Mo) 0.00178) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-09Du.tdb | 984.95 | LIQUID (x(Mo) 0.00178) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-09Du.tdb | 933.29 | FCC_A1 (x(Mo) 2.400e-4) + LIQUID (x(Mo) 5.100e-4) + AL12MO (x(Mo) 0.07692) |
| AlMo-10Cup.tdb | 3595.7 | LIQUID#2 (x(Mo) 0.20133) + BCC_A2 (x(Mo) 0.68917) + LIQUID (x(Mo) 0.93868) |
| AlMo-10Cup.tdb | 3348.11 | LIQUID#2 (x(Mo) 0.23618) + LIQUID (x(Mo) 0.6514) + BCC_A2 (x(Mo) 0.65956) |
| AlMo-10Cup.tdb | 2423.16 | LIQUID (x(Mo) 0.74525) + ALMO3_A15 (x(Mo) 0.75498) + BCC_A2 (x(Mo) 0.78902) |
| AlMo-10Cup.tdb | 1992.98 | BCC_A2 (x(Mo) 0.54402) + LIQUID (x(Mo) 0.56259) + ALMO3_A15 (x(Mo) 0.70795) |
| AlMo-10Cup.tdb | 1842.87 | LIQUID (x(Mo) 0.36855) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.44747) |
| AlMo-10Cup.tdb | 1819.5 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.30403) + AL63MO37 (x(Mo) 0.37) |
| AlMo-10Cup.tdb | 1819.5 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.30422) + AL63MO37 (x(Mo) 0.37) |
| AlMo-10Cup.tdb | 1762.73 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.47963) |
| AlMo-10Cup.tdb | 1762.73 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.47977) |
| AlMo-10Cup.tdb | 1743.14 | AL8MO3 (x(Mo) 0.27273) + BCC_A2 (x(Mo) 0.49531) + ALMO3_A15 (x(Mo) 0.70916) |
| AlMo-10Cup.tdb | 1495.16 | LIQUID (x(Mo) 0.0472) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-10Cup.tdb | 1495.16 | LIQUID (x(Mo) 0.04724) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-10Cup.tdb | 1425.16 | LIQUID (x(Mo) 0.0326) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-10Cup.tdb | 1425.16 | LIQUID (x(Mo) 0.03263) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-10Cup.tdb | 1425.16 | LIQUID (x(Mo) 0.0327) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-10Cup.tdb | 1270 | LIQUID (x(Mo) 0.01052) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-10Cup.tdb | 1270 | LIQUID (x(Mo) 0.01054) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-10Cup.tdb | 1270 | LIQUID (x(Mo) 0.01049) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-10Cup.tdb | 1215.15 | AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-10Cup.tdb | 1213.16 | LIQUID (x(Mo) 0.00607) + AL22MO5 (x(Mo) 0.18519) + AL17MO4 (x(Mo) 0.19048) |
| AlMo-10Cup.tdb | 1213.16 | LIQUID (x(Mo) 0.00605) + AL22MO5 (x(Mo) 0.18519) + AL17MO4 (x(Mo) 0.19048) |
| AlMo-10Cup.tdb | 1119.15 | LIQUID (x(Mo) 0.00209) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-10Cup.tdb | 1119.15 | LIQUID (x(Mo) 0.00209) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-10Cup.tdb | 1119.15 | LIQUID (x(Mo) 0.00209) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-10Cup.tdb | 1064.15 | AL17MO4 (x(Mo) 0.19048) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-10Cup.tdb | 985.15 | LIQUID (x(Mo) 2.800e-4) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-10Cup.tdb | 985.15 | LIQUID (x(Mo) 2.800e-4) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-10Cup.tdb | 933.88 | LIQUID (x(Mo) 7.000e-5) + FCC_A1 (x(Mo) 6.700e-4) + AL12MO (x(Mo) 0.07692) |
| AlMo-16Pen.tdb | 2420.51 | LIQUID (x(Mo) 0.66942) + ALMO3_A15 (x(Mo) 0.75488) + B2_BCC (x(Mo) 0.78874) |
| AlMo-16Pen.tdb | 1994.1 | LIQUID (x(Mo) 0.40278) + B2_BCC (x(Mo) 0.54435) + ALMO3_A15 (x(Mo) 0.70797) |
| AlMo-16Pen.tdb | 1842.46 | LIQUID (x(Mo) 0.32702) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.46835) |
| AlMo-16Pen.tdb | 1842.46 | LIQUID (x(Mo) 0.32706) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.46839) |
| AlMo-16Pen.tdb | 1801.51 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.2851) + AL63MO37 (x(Mo) 0.37) |
| AlMo-16Pen.tdb | 1801.51 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.28519) + AL63MO37 (x(Mo) 0.37) |
| AlMo-16Pen.tdb | 1801.51 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.285) + AL63MO37 (x(Mo) 0.37) |
| AlMo-16Pen.tdb | 1762.59 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.47987) |
| AlMo-16Pen.tdb | 1743.13 | AL8MO3 (x(Mo) 0.27273) + B2_BCC (x(Mo) 0.49532) + ALMO3_A15 (x(Mo) 0.70916) |
| AlMo-16Pen.tdb | 1495.02 | LIQUID (x(Mo) 0.05603) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-16Pen.tdb | 1495.02 | LIQUID (x(Mo) 0.05607) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-16Pen.tdb | 1425.24 | LIQUID (x(Mo) 0.04186) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-16Pen.tdb | 1425.24 | LIQUID (x(Mo) 0.04189) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-16Pen.tdb | 1425.24 | LIQUID (x(Mo) 0.04189) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-16Pen.tdb | 1270.43 | LIQUID (x(Mo) 0.01827) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-16Pen.tdb | 1270.43 | LIQUID (x(Mo) 0.0183) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-16Pen.tdb | 1270.43 | LIQUID (x(Mo) 0.01827) + AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) |
| AlMo-16Pen.tdb | 1214.56 | AL17MO4 (x(Mo) 0.19048) + AL4MO (x(Mo) 0.2) + AL3MO (x(Mo) 0.25) |
| AlMo-16Pen.tdb | 1213.19 | LIQUID (x(Mo) 0.01221) + AL22MO5 (x(Mo) 0.18519) + AL17MO4 (x(Mo) 0.19048) |
| AlMo-16Pen.tdb | 1213.19 | LIQUID (x(Mo) 0.01219) + AL22MO5 (x(Mo) 0.18519) + AL17MO4 (x(Mo) 0.19048) |
| AlMo-16Pen.tdb | 1118.62 | LIQUID (x(Mo) 0.00544) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-16Pen.tdb | 1118.62 | LIQUID (x(Mo) 0.00545) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-16Pen.tdb | 1118.62 | LIQUID (x(Mo) 0.00544) + AL5MO (x(Mo) 0.16667) + AL22MO5 (x(Mo) 0.18519) |
| AlMo-16Pen.tdb | 1064.56 | AL17MO4 (x(Mo) 0.19048) + AL3MO (x(Mo) 0.25) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-16Pen.tdb | 985.17 | LIQUID (x(Mo) 0.00109) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-16Pen.tdb | 985.17 | LIQUID (x(Mo) 0.00109) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-16Pen.tdb | 933.68 | LIQUID (x(Mo) 3.100e-4) + FCC_A1 (x(Mo) 6.100e-4) + AL12MO (x(Mo) 0.07692) |
| AlMo-97Cos.tdb | 2169.87 | LIQUID (x(Mo) 0.68627) + ALMO3_A15 (x(Mo) 0.75) + BCC_A2 (x(Mo) 0.85328) |
| AlMo-97Cos.tdb | 2169.87 | LIQUID (x(Mo) 0.68637) + ALMO3_A15 (x(Mo) 0.75) + BCC_A2 (x(Mo) 0.85336) |
| AlMo-97Cos.tdb | 1989.99 | ALMO_A2 (x(Mo) 0.5) + LIQUID (x(Mo) 0.55872) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Cos.tdb | 1989.99 | ALMO_A2 (x(Mo) 0.5) + LIQUID (x(Mo) 0.5588) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Cos.tdb | 1989.99 | ALMO_A2 (x(Mo) 0.5) + LIQUID (x(Mo) 0.55882) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Cos.tdb | 1810.68 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.35933) + ALMO_A2 (x(Mo) 0.5) |
| AlMo-97Cos.tdb | 1810.68 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.35939) + ALMO_A2 (x(Mo) 0.5) |
| AlMo-97Cos.tdb | 1462.8 | AL8MO3 (x(Mo) 0.27273) + ALMO_A2 (x(Mo) 0.5) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Cos.tdb | 933.33 | FCC_A1 (x(Mo) 0) + LIQUID (x(Mo) 2.200e-4) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-97Sau.tdb | 2390.35 | LIQUID (x(Mo) 0.62306) + ALMO3_A15 (x(Mo) 0.75) + BCC_A2 (x(Mo) 0.77151) |
| AlMo-97Sau.tdb | 2390.35 | LIQUID (x(Mo) 0.62319) + ALMO3_A15 (x(Mo) 0.75) + BCC_A2 (x(Mo) 0.77162) |
| AlMo-97Sau.tdb | 1920 | LIQUID (x(Mo) 0.42955) + BCC_A2 (x(Mo) 0.5375) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Sau.tdb | 1920 | LIQUID (x(Mo) 0.42955) + BCC_A2 (x(Mo) 0.53751) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Sau.tdb | 1845.43 | AL63MO37 (x(Mo) 0.37) + LIQUID (x(Mo) 0.39622) + BCC_A2 (x(Mo) 0.48669) |
| AlMo-97Sau.tdb | 1845.43 | AL63MO37 (x(Mo) 0.37) + LIQUID (x(Mo) 0.39623) + BCC_A2 (x(Mo) 0.4867) |
| AlMo-97Sau.tdb | 1836.49 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.33533) + AL63MO37 (x(Mo) 0.37) |
| AlMo-97Sau.tdb | 1836.49 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.33501) + AL63MO37 (x(Mo) 0.37) |
| AlMo-97Sau.tdb | 1762.86 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.48049) |
| AlMo-97Sau.tdb | 1762.86 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.4805) |
| AlMo-97Sau.tdb | 1762.86 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + BCC_A2 (x(Mo) 0.48049) |
| AlMo-97Sau.tdb | 1728.53 | AL8MO3 (x(Mo) 0.27273) + BCC_A2 (x(Mo) 0.49933) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Sau.tdb | 1728.53 | AL8MO3 (x(Mo) 0.27273) + BCC_A2 (x(Mo) 0.49934) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Sau.tdb | 1728.53 | AL8MO3 (x(Mo) 0.27273) + BCC_A2 (x(Mo) 0.49931) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-97Sau.tdb | 1422.14 | LIQUID (x(Mo) 0.03222) + AL4MO (x(Mo) 0.2) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-97Sau.tdb | 1422.14 | LIQUID (x(Mo) 0.03228) + AL4MO (x(Mo) 0.2) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-97Sau.tdb | 996.19 | LIQUID (x(Mo) 8.100e-4) + AL5MO (x(Mo) 0.16667) + AL4MO (x(Mo) 0.2) |
| AlMo-97Sau.tdb | 996.19 | LIQUID (x(Mo) 8.100e-4) + AL5MO (x(Mo) 0.16667) + AL4MO (x(Mo) 0.2) |
| AlMo-97Sau.tdb | 996.19 | LIQUID (x(Mo) 8.100e-4) + AL5MO (x(Mo) 0.16667) + AL4MO (x(Mo) 0.2) |
| AlMo-97Sau.tdb | 971.59 | LIQUID (x(Mo) 5.700e-4) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-97Sau.tdb | 971.59 | LIQUID (x(Mo) 5.700e-4) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-97Sau.tdb | 934 | LIQUID (x(Mo) 2.200e-4) + FCC_A1 (x(Mo) 9.900e-4) + AL12MO (x(Mo) 0.07692) |
| AlMo-98Sau-LB.tdb | 2418.93 | LIQUID (x(Mo) 0.62053) + ALMO3_A15 (x(Mo) 0.75) + B2_BCC (x(Mo) 0.79061) |
| AlMo-98Sau-LB.tdb | 2418.93 | LIQUID (x(Mo) 0.62067) + ALMO3_A15 (x(Mo) 0.75) + B2_BCC (x(Mo) 0.7907) |
| AlMo-98Sau-LB.tdb | 2418.93 | LIQUID (x(Mo) 0.62067) + ALMO3_A15 (x(Mo) 0.75) + BCC_A2 (x(Mo) 0.7907) |
| AlMo-98Sau-LB.tdb | 1976.91 | LIQUID (x(Mo) 0.41537) + B2_BCC (x(Mo) 0.53257) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-98Sau-LB.tdb | 1976.91 | LIQUID (x(Mo) 0.41541) + B2_BCC (x(Mo) 0.53261) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-98Sau-LB.tdb | 1976.91 | LIQUID (x(Mo) 0.41541) + B2_BCC (x(Mo) 0.53261) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-98Sau-LB.tdb | 1844.43 | LIQUID (x(Mo) 0.35688) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.49561) |
| AlMo-98Sau-LB.tdb | 1844.43 | LIQUID (x(Mo) 0.35691) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.49563) |
| AlMo-98Sau-LB.tdb | 1844.43 | LIQUID (x(Mo) 0.35691) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.49563) |
| AlMo-98Sau-LB.tdb | 1836.41 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.33269) + AL63MO37 (x(Mo) 0.37) |
| AlMo-98Sau-LB.tdb | 1836.41 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.33321) + AL63MO37 (x(Mo) 0.37) |
| AlMo-98Sau-LB.tdb | 1836.41 | AL8MO3 (x(Mo) 0.27273) + LIQUID (x(Mo) 0.33249) + AL63MO37 (x(Mo) 0.37) |
| AlMo-98Sau-LB.tdb | 1765.57 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.5061) |
| AlMo-98Sau-LB.tdb | 1765.57 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.5062) |
| AlMo-98Sau-LB.tdb | 1765.57 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.50617) |
| AlMo-98Sau-LB.tdb | 1765.57 | AL8MO3 (x(Mo) 0.27273) + AL63MO37 (x(Mo) 0.37) + B2_BCC (x(Mo) 0.5062) |
| AlMo-98Sau-LB.tdb | 1739.78 | AL8MO3 (x(Mo) 0.27273) + B2_BCC (x(Mo) 0.51254) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-98Sau-LB.tdb | 1739.78 | AL8MO3 (x(Mo) 0.27273) + B2_BCC (x(Mo) 0.51261) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-98Sau-LB.tdb | 1739.78 | AL8MO3 (x(Mo) 0.27273) + B2_BCC (x(Mo) 0.51252) + ALMO3_A15 (x(Mo) 0.75) |
| AlMo-98Sau-LB.tdb | 1397.72 | LIQUID (x(Mo) 0.02834) + AL4MO (x(Mo) 0.2) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-98Sau-LB.tdb | 1397.72 | LIQUID (x(Mo) 0.02836) + AL4MO (x(Mo) 0.2) + AL8MO3 (x(Mo) 0.27273) |
| AlMo-98Sau-LB.tdb | 1025.24 | LIQUID (x(Mo) 0.00121) + AL5MO (x(Mo) 0.16667) + AL4MO (x(Mo) 0.2) |
| AlMo-98Sau-LB.tdb | 1025.24 | LIQUID (x(Mo) 0.00121) + AL5MO (x(Mo) 0.16667) + AL4MO (x(Mo) 0.2) |
| AlMo-98Sau-LB.tdb | 1025.24 | LIQUID (x(Mo) 0.00121) + AL5MO (x(Mo) 0.16667) + AL4MO (x(Mo) 0.2) |
| AlMo-98Sau-LB.tdb | 971.63 | LIQUID (x(Mo) 5.700e-4) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-98Sau-LB.tdb | 971.63 | LIQUID (x(Mo) 5.700e-4) + AL12MO (x(Mo) 0.07692) + AL5MO (x(Mo) 0.16667) |
| AlMo-98Sau-LB.tdb | 933.82 | LIQUID (x(Mo) 2.200e-4) + FCC_A1 (x(Mo) 7.200e-4) + AL12MO (x(Mo) 0.07692) |
| AlMo-98Sau-LB.tdb | 332.1 | AL5MO (x(Mo) 0.16667) + AL4MO (x(Mo) 0.2) + AL8MO3 (x(Mo) 0.27273) |

Convex hulls: [Materials Project DFT hull](https://data.orchid-project.org/hulls/dft-mp/AL/AL-MO.json) · [OQMD DFT hull](https://data.orchid-project.org/hulls/dft-oqmd/AL/AL-MO.json) · [CALPHAD hull AlMo-09Du](https://data.orchid-project.org/hulls/calphad-sgte/AL/AL-MO--AlMo-09Du.json) · [CALPHAD hull AlMo-10Cup](https://data.orchid-project.org/hulls/calphad-sgte/AL/AL-MO--AlMo-10Cup.json) · [CALPHAD hull AlMo-97Cos](https://data.orchid-project.org/hulls/calphad-sgte/AL/AL-MO--AlMo-97Cos.json) · [CALPHAD hull AlMo-97Sau](https://data.orchid-project.org/hulls/calphad-sgte/AL/AL-MO--AlMo-97Sau.json) · [CALPHAD hull AlMo-98Sau-LB](https://data.orchid-project.org/hulls/calphad-sgte/AL/AL-MO--AlMo-98Sau-LB.json)

## Invariant reactions (literature)

Table: Invariant reactions reported in the literature for the Al–Mo system (94)

| T (K) | Reaction / phases | Compositions (mole fraction) | Class | Source | Location | Quote |
|---:|---|---|---|---|---|---|
| 2896.15 | congruent melting: Mo \<-> L | Mo: Mo 1 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 13; `ORC-TMWO3RWT5X` |  |
| 2423.15 | peritectic: L + (Mo) \<-> AlMo3 | L: Mo 0.65; (Mo): Mo 0.795; AlMo3: Mo 0.75 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 12; `ORC-EEGMWMZITS` |  |
| 2423 | liq. + bcc(Mo) -> AlMo3 | bcc(Mo): Mo 0.81; AlMo3: Mo 0.755 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 2; `ORC-HATKYHLV7P` |  |
| 2423 | liq. + bcc(Mo) -> AlMo3 | L: Mo 0.7155; bcc(Mo): Mo 0.7767; AlMo3: Mo 0.752 | model | [2] Du 2009 | Table 2, p. 7, row 1; `ORC-L2VOEPDVK6` |  |
| 2423 | Liquid + β -> δ-AlMo3 | Liquid: Al 0.3; β: Al 0.195; δ-AlMo3: Al 0.25 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 1; `ORC-MDBPKSJ3TT` |  |
| 2423 | Liquid + β -> δ-AlMo3 | Liquid: Al 0.255; β: Al 0.211; δ-AlMo3: Al 0.245 | model | [3] Cupid 2010 | Table 2, p. 6, row 3; `ORC-MH5J4J4AII` |  |
| 2423 | Liquid + β -> δ-AlMo3 | δ-AlMo3: Al 0.25, Mo 0.75 | experimental | [3] Cupid 2010; _cites Ham 1951_ | Table 2, p. 6, row 2; `ORC-YFFFSQ42EQ` |  |
| 2023 | congruent melting: Liquid -> AlMo | Liquid: Al 0.5; AlMo: Al 0.5 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 4; `ORC-OIOA3PT3GM` |  |
| 2023 | congruent melting: Liquid -> AlMo | Liquid: Al 0.484; AlMo: Al 0.484 | model | [3] Cupid 2010 | Table 2, p. 6, row 5; `ORC-Z57I75NBHJ` |  |
| 1993.15 | peritectic: L + AlMo3 \<-> AlMo | L: Mo 0.45; AlMo3: Mo 0.73; AlMo: Mo 0.54 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 11; `ORC-XK222FP4IA` |  |
| 1993 | eutectic: Liquid -> δ-AlMo3 + AlMo | Liquid: Al 0.437; δ-AlMo3: Al 0.292; AlMo: Al 0.456 | model | [3] Cupid 2010 | Table 2, p. 6, row 8; `ORC-5TD63XPCXU` |  |
| 1993 | liq. + AlMo3 -> AlMo | L: Mo 0.4378; AlMo3: Mo 0.7315; AlMo: Mo 0.5523 | model | [2] Du 2009 | Table 2, p. 7, row 3; `ORC-CEIYUT43N6` |  |
| 1993 | eutectic: Liquid -> δ-AlMo3 + AlMo | δ-AlMo3: Al 0.25, Mo 0.75; AlMo: Al 0.5, Mo 0.5 | experimental | [3] Cupid 2010; _cites Rexer 1971_ | Table 2, p. 6, row 7; `ORC-ONG5OVQRRL` |  |
| 1993 | liq. + AlMo3 -> AlMo | L: Mo 0.45; AlMo3: Mo 0.74; AlMo: Mo 0.54 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 4; `ORC-OO3PJOFRE7` |  |
| 1993 | eutectic: Liquid -> δ-AlMo3 + AlMo | Liquid: Al 0.37; δ-AlMo3: Al 0.285; AlMo: Al 0.46 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 6; `ORC-UZRAGDAEBV` |  |
| 1850.15 | congruent melting: L \<-> Al8Mo3 | L: Mo 0.273; Al8Mo3: Mo 0.273 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 9; `ORC-2HH557BSSV` |  |
| 1843.15 | peritectic: L + AlMo \<-> Al63Mo37 | L: Mo 0.35; AlMo: Mo 0.48; Al63Mo37: Mo 0.37 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 10; `ORC-QJBWH34JEL` |  |
| 1843 | Liquid + AlMo -> Al63Mo37 | Liquid: Al 0.66; AlMo: Al 0.52; Al63Mo37: Al 0.63 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 9; `ORC-DNFTPXDVSW` |  |
| 1843 | Liquid + AlMo -> Al63Mo37 | Liquid: Al 0.631; AlMo: Al 0.553; Al63Mo37: Al 0.63 | model | [3] Cupid 2010 | Table 2, p. 6, row 11; `ORC-LI6QSBNWRA` |  |
| 1843 | liq. + AlMo -> Al63Mo37 | L: Mo 0.3546; AlMo: Mo 0.4802; Al63Mo37: Al 0.63, Mo 0.37 | model | [2] Du 2009 | Table 2, p. 7, row 5; `ORC-LM5GWITZVJ` |  |
| 1843 | liq. + AlMo -> Al63Mo37 | L: Mo 0.35; AlMo: Mo 0.475; Al63Mo37: Al 0.63, Mo 0.37 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 6; `ORC-MJCPTP2HDG` |  |
| 1843 | Liquid + AlMo -> Al63Mo37 | AlMo: Al 0.5, Mo 0.5; Al63Mo37: Al 0.63, Mo 0.37 | experimental | [3] Cupid 2010; _cites Rexer 1971_ | Table 2, p. 6, row 10; `ORC-UKLQTNEFEW` |  |
| 1828 | congruent melting: Liquid -> Al8Mo3 | Liquid: Al 0.727; Al8Mo3: Al 0.727 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 12; `ORC-OQBYI4WXFI` |  |
| 1821 | congruent melting: Liquid -> Al8Mo3 | Liquid: Al 0.727; Al8Mo3: Al 0.727 | model | [3] Cupid 2010 | Table 2, p. 6, row 14; `ORC-EFIZPZSYCM` |  |
| 1819 | eutectic: Liquid -> Al63Mo37 + Al8Mo3 | Liquid: Al 0.696; Al63Mo37: Al 0.63; Al8Mo3: Al 0.727 | model | [3] Cupid 2010 | Table 2, p. 6, row 17; `ORC-4XRFMMMULS` |  |
| 1819 | congruent melting: liq. -> Al8Mo3 | L: Al 0.727273, Mo 0.272727; Al8Mo3: Al 0.727273, Mo 0.272727 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 14; `ORC-6WETZ4LDME` |  |
| 1819 | congruent melting: Liquid -> Al8Mo3 | Liquid: Al 0.727273, Mo 0.272727; Al8Mo3: Al 0.727273, Mo 0.272727 | unspecified | [3] Cupid 2010; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 6, row 13; `ORC-OC3KJZEJNF` |  |
| 1819 | congruent melting: liq. -> Al8Mo3 | L: Al 0.727273, Mo 0.272727; Al8Mo3: Al 0.727273, Mo 0.272727 | model | [2] Du 2009 | Table 2, p. 7, row 13; `ORC-PKXSXHBWGZ` |  |
| 1814 | eutectic: liq. -> Al8Mo3 + Al63Mo37 | L: Mo 0.3083; Al8Mo3: Al 0.727273, Mo 0.272727; Al63Mo37: Al 0.63, Mo 0.37 | model | [2] Du 2009 | Table 2, p. 7, row 7; `ORC-LPFGEDFC3G` |  |
| 1808.15 | eutectic: L \<-> Al8Mo3 + Al63Mo37 | L: Mo 0.285; Al8Mo3: Mo 0.278; Al63Mo37: Mo 0.37 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 8; `ORC-SC7VI3B4K6` |  |
| 1808 | eutectic: Liquid -> Al63Mo37 + Al8Mo3 | Liquid: Al 0.715; Al63Mo37: Al 0.63; Al8Mo3: Al 0.727 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 15; `ORC-6O2UNF2ONY` |  |
| 1808 | eutectic: liq. -> Al8Mo3 + Al63Mo37 | L: Mo 0.32; Al8Mo3: Al 0.727273, Mo 0.272727; Al63Mo37: Al 0.63, Mo 0.37 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 8; `ORC-7UT5UWTBTD` |  |
| 1808 | eutectic: Liquid -> Al63Mo37 + Al8Mo3 | Al63Mo37: Al 0.63, Mo 0.37; Al8Mo3: Al 0.727273, Mo 0.272727 | experimental | [3] Cupid 2010; _cites Rexer 1971_ | Table 2, p. 6, row 16; `ORC-VGJK25FWKY` |  |
| 1763.15 | eutectoid: Al63Mo37 \<-> Al8Mo3 + AlMo | Al63Mo37: Mo 0.37; Al8Mo3: Mo 0.286; AlMo: Mo 0.495 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 7; `ORC-NZILDOLYCE` |  |
| 1763 | Al63Mo37 -> Al8Mo3 + AlMo | Al63Mo37: Al 0.63, Mo 0.37; Al8Mo3: Al 0.727273, Mo 0.272727; AlMo: Mo 0.4818 | model | [2] Du 2009 | Table 2, p. 7, row 9; `ORC-6WJHXJ67TX` |  |
| 1763 | Al63Mo37 -> AlMo + Al8Mo3 | Al63Mo37: Al 0.63, Mo 0.37; AlMo: Al 0.5, Mo 0.5; Al8Mo3: Al 0.727273, Mo 0.272727 | experimental | [3] Cupid 2010; _cites Rexer 1971_ | Table 2, p. 6, row 19; `ORC-EBGO3EI5UM` |  |
| 1763 | Al63Mo37 -> AlMo + Al8Mo3 | Al63Mo37: Al 0.63; AlMo: Al 0.52; Al8Mo3: Al 0.727 | model | [3] Cupid 2010 | Table 2, p. 6, row 20; `ORC-LII7XD5A6E` |  |
| 1763 | Al63Mo37 -> AlMo + Al8Mo3 | Al63Mo37: Al 0.63; AlMo: Al 0.505; Al8Mo3: Al 0.727 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 18; `ORC-ULCBDIHZOX` |  |
| 1763 | Al63Mo37 -> Al8Mo3 + AlMo | Al63Mo37: Al 0.63, Mo 0.37; Al8Mo3: Al 0.727273, Mo 0.272727; AlMo: Mo 0.49 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 10; `ORC-VCFQLYAA2H` |  |
| 1743.15 | eutectoid: AlMo \<-> Al8Mo3 + AlMo3 | AlMo: Mo 0.5; Al8Mo3: Mo 0.287; AlMo3: Mo 0.725 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 6; `ORC-ZFMKYMNMM2` |  |
| 1743 | AlMo -> δ-AlMo3 + Al8Mo3 | AlMo: Al 0.5; δ-AlMo3: Al 0.27; Al8Mo3: Al 0.727 | unspecified | [3] Cupid 2010; _cites Schuster 2003_ | Table 2, p. 6, row 21; `ORC-65WXPPDOY6` |  |
| 1743 | AlMo -> Al8Mo3 + AlMo3 | AlMo: Mo 0.5; Al8Mo3: Al 0.727273, Mo 0.272727; AlMo3: Mo 0.74 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 12; `ORC-FCSX2GDIF5` |  |
| 1743 | AlMo -> δ-AlMo3 + Al8Mo3 | AlMo: Al 0.5, Mo 0.5; δ-AlMo3: Al 0.25, Mo 0.75; Al8Mo3: Al 0.727273, Mo 0.272727 | experimental | [3] Cupid 2010; _cites Rexer 1971_ | Table 2, p. 6, row 22; `ORC-J6FVTSOC57` |  |
| 1743 | AlMo -> δ-AlMo3 + Al8Mo3 | AlMo: Al 0.505; δ-AlMo3: Al 0.291; Al8Mo3: Al 0.727 | model | [3] Cupid 2010 | Table 2, p. 6, row 23; `ORC-MG4EN7LCLJ` |  |
| 1743 | AlMo -> Al8Mo3 + AlMo3 | AlMo: Mo 0.4914; Al8Mo3: Al 0.727273, Mo 0.272727; AlMo3: Mo 0.7331 | model | [2] Du 2009 | Table 2, p. 7, row 11; `ORC-QYJH2C5CMP` |  |
| 1495 | eutectic: liq. -> Al8Mo3 + Al3Mo | L: Mo 0.0582; Al8Mo3: Al 0.727273, Mo 0.272727; Al3Mo: Al 0.75, Mo 0.25 | model | [2] Du 2009 | Table 2, p. 7, row 15; `ORC-HPTIQ2LLEY` |  |
| 1495 | Liquid + Al8Mo3 -> Al3Mo | Al8Mo3: Al 0.727273, Mo 0.272727; Al3Mo: Al 0.75, Mo 0.25 | unspecified | [3] Cupid 2010; _cites Schuster 1991_ [doi](https://doi.org/10.1007/bf02646496) | Table 2, p. 6, row 24; `ORC-PVH4XY5DT6` |  |
| 1495 | eutectic: liq. -> Al8Mo3 + Al3Mo | L: Mo 0.055; Al8Mo3: Al 0.727273, Mo 0.272727; Al3Mo: Al 0.75, Mo 0.25 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 16; `ORC-YZFXHWMMAJ` |  |
| 1495 | Liquid + Al8Mo3 -> Al3Mo | Liquid: Al 0.953; Al8Mo3: Al 0.727273, Mo 0.272727; Al3Mo: Al 0.75, Mo 0.25 | model | [3] Cupid 2010 | Table 2, p. 6, row 25; `ORC-Z3NJU4LRUE` |  |
| 1425 | liq. + Al3Mo -> Al4Mo | Al3Mo: Mo 0.0227; Al4Mo: Al 0.8, Mo 0.2 | model | [2] Du 2009 | Table 2, p. 7, row 17; `ORC-2NYZ2BDEXB` |  |
| 1425 | Liquid + Al3Mo -> Al4Mo | Al3Mo: Al 0.75, Mo 0.25; Al4Mo: Al 0.8, Mo 0.2 | unspecified | [3] Cupid 2010; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 6, row 26; `ORC-CICYCSEDNJ` |  |
| 1425 | Liquid + Al3Mo -> Al4Mo | Liquid: Al 0.967; Al3Mo: Al 0.75, Mo 0.25; Al4Mo: Al 0.8, Mo 0.2 | model | [3] Cupid 2010 | Table 2, p. 6, row 27; `ORC-MK7TF4PSDT` |  |
| 1425 | liq. + Al3Mo -> Al4Mo | Al3Mo: Mo 0.035; Al4Mo: Al 0.8, Mo 0.2 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 18; `ORC-ULLOJ34JU4` |  |
| 1403.15 | peritectic: L + Al8Mo3 \<-> Al4Mo | L: Mo 0.03; Al8Mo3: Mo 0.255; Al4Mo: Mo 0.2 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 5; `ORC-7AGIL3SUKL` |  |
| 1403.15 | peritectic |  | experimental | [1] Ltd. 1997; _cites E Spemer 1959_ | p. 1; `ORC-AZTBPIOYPX` | “\[59Spe\] reported the peritectic formation of AlaMo from AI2Mo at 1130 ~ and the congruent melting of AI2Mo at -2000 ~” |
| 1403 | peritectic |  | experimental | [3] Cupid 2010 | p. 2; `ORC-RSMOFFZ24G.27a810` | “Al3Mo was shown to form peritectically at 1403 K and Al2Mo was shown to melt congruently at z2323 K.” |
| 1273 | liq. + Al4Mo -> Al17Mo4 | L: Mo 0.03; Al4Mo: Al 0.8, Mo 0.2; Al17Mo4: Al 0.809524, Mo 0.190476 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 20; `ORC-2DXSRN7IMW` |  |
| 1273 | Liquid + Al4Mo -> Al17Mo4 | Al4Mo: Al 0.8, Mo 0.2; Al17Mo4: Al 0.809524, Mo 0.190476 | unspecified | [3] Cupid 2010; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 6, row 28; `ORC-L2DLPX73DB` |  |
| 1270 | Liquid + Al4Mo -> Al17Mo4 | Liquid: Al 0.995; Al4Mo: Al 0.8, Mo 0.2; Al17Mo4: Al 0.809524, Mo 0.190476 | model | [3] Cupid 2010 | Table 2, p. 6, row 29; `ORC-TU3VEUFVCG` |  |
| 1267 | liq. + Al4Mo -> Al17Mo4 | L: Mo 0.0227; Al4Mo: Al 0.8, Mo 0.2; Al17Mo4: Al 0.809524, Mo 0.190476 | model | [2] Du 2009 | Table 2, p. 7, row 19; `ORC-G4ZSJXD6Y4` |  |
| 1223 | Liquid + Al17Mo4 -> Al22Mo5 | Al17Mo4: Al 0.809524, Mo 0.190476; Al22Mo5: Al 0.814815, Mo 0.185185 | unspecified | [3] Cupid 2010; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 6, row 32; `ORC-JV4QYU4UGB` |  |
| 1223 | liq. + Al17Mo4 -> Al22Mo5 | L: Mo 0.02; Al17Mo4: Al 0.809524, Mo 0.190476; Al22Mo5: Al 0.814815, Mo 0.185185 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 22; `ORC-YODDT2ZUD7` |  |
| 1218 | liq. + Al17Mo4 -> Al22Mo5 | L: Mo 0.0168; Al17Mo4: Al 0.809524, Mo 0.190476; Al22Mo5: Al 0.814815, Mo 0.185185 | model | [2] Du 2009 | Table 2, p. 7, row 21; `ORC-QU66SM53G4` |  |
| 1215 | Al4Mo -> Al3Mo + Al17Mo4 | Al4Mo: Al 0.8, Mo 0.2; Al3Mo: Al 0.75, Mo 0.25; Al17Mo4: Al 0.809524, Mo 0.190476 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 24; `ORC-5TX3NSHV24` |  |
| 1215 | Al4Mo -> Al3Mo + Al17Mo4 | Al4Mo: Al 0.8, Mo 0.2; Al3Mo: Al 0.75, Mo 0.25; Al17Mo4: Al 0.809524, Mo 0.190476 | model | [2] Du 2009 | Table 2, p. 7, row 23; `ORC-ET5WAAF3EY` |  |
| 1215 | Al4Mo -> Al3Mo + Al17Mo4 | Al4Mo: Al 0.8, Mo 0.2; Al3Mo: Al 0.75, Mo 0.25; Al17Mo4: Al 0.809524, Mo 0.190476 | unspecified | [3] Cupid 2010; _cites Schuster 1991_ [doi](https://doi.org/10.1007/bf02646496) | Table 2, p. 6, row 30; `ORC-O3OWCUECML` |  |
| 1215 | Al4Mo -> Al3Mo + Al17Mo4 | Al4Mo: Al 0.8, Mo 0.2; Al3Mo: Al 0.75, Mo 0.25; Al17Mo4: Al 0.809524, Mo 0.190476 | model | [3] Cupid 2010 | Table 2, p. 6, row 31; `ORC-WZ7267EOTV` |  |
| 1213 | Liquid + Al17Mo4 -> Al22Mo5 | Liquid: Al 0.994; Al17Mo4: Al 0.809524, Mo 0.190476; Al22Mo5: Al 0.814815, Mo 0.185185 | model | [3] Cupid 2010 | Table 2, p. 6, row 33; `ORC-STCK4LNW2N` |  |
| 1119 | Liquid + Al22Mo5 -> Al5Mo | Al22Mo5: Al 0.814815, Mo 0.185185; Al5Mo: Al 0.833333, Mo 0.166667 | unspecified | [3] Cupid 2010; _cites Schuster 1991_ [doi](https://doi.org/10.1007/bf02646496) | Table 2, p. 6, row 34; `ORC-5LTXFBFTVU` |  |
| 1119 | liq. + Al22Mo5 -> Al5Mo | L: Mo 0.01; Al22Mo5: Al 0.814815, Mo 0.185185; Al5Mo: Al 0.833333, Mo 0.166667 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 26; `ORC-G3FPDORWQQ` |  |
| 1119 | Liquid + Al22Mo5 -> Al5Mo | Liquid: Al 0.998; Al22Mo5: Al 0.814815, Mo 0.185185; Al5Mo: Al 0.833333, Mo 0.166667 | model | [3] Cupid 2010 | Table 2, p. 6, row 35; `ORC-MREUMLKTS4` |  |
| 1119 | liq. + Al22Mo5 -> Al5Mo | L: Mo 0.0079; Al22Mo5: Al 0.814815, Mo 0.185185; Al5Mo: Al 0.833333, Mo 0.166667 | model | [2] Du 2009 | Table 2, p. 7, row 25; `ORC-UEM5DG4ROO` |  |
| 1073 | Al3Mo -> Al8Mo3 + Al17Mo4 | Al3Mo: Al 0.75, Mo 0.25; Al8Mo3: Al 0.727273, Mo 0.272727; Al17Mo4: Al 0.809524, Mo 0.190476 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 28; `ORC-DZMLVD5APX` |  |
| 1073 | Al3Mo -> Al8Mo3 + Al17Mo4 | Al3Mo: Al 0.75, Mo 0.25; Al8Mo3: Al 0.727273, Mo 0.272727; Al17Mo4: Al 0.809524, Mo 0.190476 | unspecified | [3] Cupid 2010; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 6, row 36; `ORC-NCVZWF3XRJ` |  |
| 1064 | Al3Mo -> Al8Mo3 + Al17Mo4 | Al3Mo: Al 0.75, Mo 0.25; Al8Mo3: Al 0.727273, Mo 0.272727; Al17Mo4: Al 0.809524, Mo 0.190476 | model | [3] Cupid 2010 | Table 2, p. 6, row 37; `ORC-BW7FX7PUHJ` |  |
| 1017 | Al3Mo -> Al8Mo3 + Al17Mo4 | Al3Mo: Al 0.75, Mo 0.25; Al8Mo3: Al 0.727273, Mo 0.272727; Al17Mo4: Al 0.809524, Mo 0.190476 | model | [2] Du 2009 | Table 2, p. 7, row 27; `ORC-GPBLVII3ZP` |  |
| 1008.15 | peritectic: L + Al4Mo \<-> Al5Mo | L: Mo 0.001; Al4Mo: Mo 0.2; Al5Mo: Mo 0.167 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 4; `ORC-MEKGNXHCDG` |  |
| 1008 | peritectic |  | experimental | [3] Cupid 2010; _cites Sperner 1959_ | p. 2; `ORC-EGUG55F6SN.befdc0` | “The peritectic formation of Al5Mo was measured at 976 K \[26\], 1008 K \[22\], and 990 K \[25\], respectively.” |
| 1008 | peritectic |  | experimental | [3] Cupid 2010; _cites Reimann 1922_ | p. 2; `ORC-ZF373L6HEO` | “Reimann \[28\] confirmed the peritectic formation of Al4Mo through microstructural investigation of a 12 wt.%Mo ascast alloy and, using DTA, measured its peritectic formation temperature as 1008 K.” |
| 990 | peritectic |  | experimental | [3] Cupid 2010; _cites Kamei 1972_ | p. 2; `ORC-EGUG55F6SN.4d0ede` | “The peritectic formation of Al5Mo was measured at 976 K \[26\], 1008 K \[22\], and 990 K \[25\], respectively.” |
| 985 | liq. + Al5Mo -> Al12Mo | L: Mo 0.0018; Al5Mo: Al 0.833333, Mo 0.166667; Al12Mo: Al 0.923077, Mo 0.076923 | model | [2] Du 2009 | Table 2, p. 7, row 29; `ORC-2TG5WQBF6K` |  |
| 985 | Liquid + Al5Mo -> Al12Mo | Al5Mo: Al 0.833333, Mo 0.166667; Al12Mo: Al 0.923077, Mo 0.076923 | unspecified | [3] Cupid 2010; _cites Schuster 1991_ [doi](https://doi.org/10.1007/bf02646496) | Table 2, p. 6, row 38; `ORC-6RV7L4QCIX` |  |
| 985 | liq. + Al5Mo -> Al12Mo | L: Mo 0.005; Al5Mo: Al 0.833333, Mo 0.166667; Al12Mo: Al 0.923077, Mo 0.076923 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 30; `ORC-BHO4ADA6SV` |  |
| 985 | Liquid + Al5Mo -> Al12Mo | Liquid: Al 0.9997; Al5Mo: Al 0.833333, Mo 0.166667; Al12Mo: Al 0.923077, Mo 0.076923 | model | [3] Cupid 2010 | Table 2, p. 6, row 39; `ORC-UDOOMVU6AN` |  |
| 976 | peritectic |  | experimental | [3] Cupid 2010; _cites Yamaguchi 1940_ | p. 2; `ORC-EGUG55F6SN.9eb2e7` | “The peritectic formation of Al5Mo was measured at 976 K \[26\], 1008 K \[22\], and 990 K \[25\], respectively.” |
| 976 | peritectic |  | experimental | [3] Cupid 2010; _cites Clare 1960_ | p. 2; `ORC-KXDZTJMGZT.9fb671` | “Al12Mo was also confirmed in the works of Sperner \[22\], Clare \[23\], Pötzschke and Schubert \[24\], and Kamei \[25\] and its peritectic formation temperature was measured at 973 K \[22\], 976 K \[23\], and 957 K \[25\], respectively.” |
| 973.15 | peritectic |  | experimental | [1] Ltd. 1997; _cites E Spemer 1959_ | p. 1; `ORC-EVKLZD62RF.19c42d` | “A review of the literature shows that the peritectic at 700 ~ is associated with the formation of All2MO \[59Spe, 60Cla, 72Kam\] and the peritectic at 735 ~ with AIsMo \[52Wac, 59Spe, 72Kam\].” |
| 973.15 | peritectic: L + Al5Mo \<-> Al12Mo | L: Mo 7.000e-4; Al5Mo: Mo 0.167; Al12Mo: Mo 0.077 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 3; `ORC-MJV2YAQP3P` |  |
| 973 | peritectic |  | experimental | [3] Cupid 2010; _cites Sperner 1959_ | p. 2; `ORC-KXDZTJMGZT.ce39d2` | “Al12Mo was also confirmed in the works of Sperner \[22\], Clare \[23\], Pötzschke and Schubert \[24\], and Kamei \[25\] and its peritectic formation temperature was measured at 973 K \[22\], 976 K \[23\], and 957 K \[25\], respectively.” |
| 957 | peritectic |  | experimental | [3] Cupid 2010; _cites Kamei 1972_ | p. 2; `ORC-KXDZTJMGZT.9fba8f` | “Al12Mo was also confirmed in the works of Sperner \[22\], Clare \[23\], Pötzschke and Schubert \[24\], and Kamei \[25\] and its peritectic formation temperature was measured at 973 K \[22\], 976 K \[23\], and 957 K \[25\], respectively.” |
| 934.15 | peritectic: L + Al12Mo \<-> (Al) | L: Mo 3.000e-4; Al12Mo: Mo 0.077; (Al): Mo 0.0064 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 2; `ORC-CWIT74WJF2` |  |
| 933.6 | congruent melting: Al \<-> L | Al: Mo 0 | unspecified | [1] Ltd. 1997 | Table 1, p. 1, row 1; `ORC-SPQ7U5NZOR` |  |
| 933 | eutectic: liq. -> Al12Mo + fcc | L: Mo 5.000e-4; Al12Mo: Al 0.923077, Mo 0.076923 | model | [2] Du 2009 | Table 2, p. 7, row 31; `ORC-3OVQYCO3PM` |  |
| 933 | eutectic: liq. -> Al12Mo + fcc | L: Mo 0.002; Al12Mo: Al 0.923077, Mo 0.076923 | experimental | [2] Du 2009; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | Table 2, p. 7, row 32; `ORC-O4FKHJOIYR` |  |

## Formation enthalpies

Literature values in kJ/mol-atom where the per-atom basis is known. DFT columns: the lowest-energy entry at the same composition (Materials Project 2026.04.13, OQMD v1.8; different energy references, never averaged), from [dft_parity.json](https://data.orchid-project.org/literature/dft_parity.json).

Table: Enthalpies of formation, Al–Mo system (29)

| Phase | Compound | Value | T (K) | Class | MP DFT (kJ/mol-atom) | OQMD DFT (kJ/mol-atom) | Source | Location | Quote |
|---|---|---:|---:|---|---:|---:|---|---|---|
| Al8Mo3 | [Al8Mo3](https://data.orchid-project.org/compounds/Al8Mo3.html) | -39.29 kJ/mol-atom | 298.15 | experimental | -32.395 (mp-aaaaaebd) | -32.317 (oqmd-10509) | [1] Ltd. 1997; _cites ref. 82Shi_ | Table 6, p. 5, row 1; `ORC-F4B3OTAYUF` |  |
| Al8Mo3 | [Al8Mo3](https://data.orchid-project.org/compounds/Al8Mo3.html) | -35.47 kJ/mol-atom |  | model | -32.395 (mp-aaaaaebd) | -32.317 (oqmd-10509) | [1] Ltd. 1997 | Table 6, p. 5, row 2; `ORC-OIUHYH55NC` |  |
| AlMo | [AlMo](https://data.orchid-project.org/compounds/AlMo.html) | -31.32 kJ/mol-atom | 298.15 | experimental |  | -18.854 (oqmd-2037612) | [1] Ltd. 1997; _cites ref. 82Shi_ | Table 6, p. 5, row 3; `ORC-2JLSMBWDJ7` |  |
| AlMo | [AlMo](https://data.orchid-project.org/compounds/AlMo.html) | -16.21 kJ/mol-atom |  | model |  | -18.854 (oqmd-2037612) | [1] Ltd. 1997 | Table 6, p. 5, row 4; `ORC-R3BGTDGYPC` |  |
| AlMo3 | [AlMo3](https://data.orchid-project.org/compounds/AlMo3.html) | -25.25 kJ/mol-atom |  | model | -23.552 (mp-aaaaaajz) | -22.704 (oqmd-10507) | [1] Ltd. 1997 | Table 6, p. 5, row 6; `ORC-MW24J4WF6Z` |  |
| AlMo3 | [AlMo3](https://data.orchid-project.org/compounds/AlMo3.html) | -21.44 kJ/mol-atom | 298.15 | experimental | -23.552 (mp-aaaaaajz) | -22.704 (oqmd-10507) | [1] Ltd. 1997; _cites ref. 82Shi_ | Table 6, p. 5, row 5; `ORC-MI42HTWPQQ` |  |
| Mo |  | -9.23 kJ/mol-atom | 298.15 | experimental |  |  | [1] Ltd. 1997; _cites ref. 82Shi_ | Table 6, p. 5, row 7; `ORC-WB6A2TW7J5` |  |
| Mo |  | -8.39 kJ/mol-atom |  | model |  |  | [1] Ltd. 1997 | Table 6, p. 5, row 8; `ORC-3F6GX5GQPZ` |  |
| Mo |  | -7.16 kJ/mol-atom | 298.15 | experimental |  |  | [1] Ltd. 1997; _cites ref. 82Shi_ | Table 6, p. 5, row 9; `ORC-DOPZG3LPKM` |  |
| Mo |  | -6.51 kJ/mol-atom |  | model |  |  | [1] Ltd. 1997 | Table 6, p. 5, row 10; `ORC-2ACGPUYHNT` |  |
| Mo |  | -4.06 kJ/mol-atom | 298.15 | experimental |  |  | [1] Ltd. 1997; _cites ref. 82Shi_ | Table 6, p. 5, row 11; `ORC-LUXPZJSFOU` |  |
| Mo |  | -3.55 kJ/mol-atom |  | model |  |  | [1] Ltd. 1997 | Table 6, p. 5, row 12; `ORC-3CEYSDAZ3F` |  |
| Mo |  | -2.26 kJ/mol-atom | 298.15 | experimental |  |  | [1] Ltd. 1997; _cites ref. 82Shi_ | Table 6, p. 5, row 13; `ORC-R6GYDE2BV5` |  |
| Mo |  | -1.86 kJ/mol-atom |  | model |  |  | [1] Ltd. 1997 | Table 6, p. 5, row 14; `ORC-QXS2DT76ZM` |  |
| Mo5Al3-D8m | [Al3Mo5](https://data.orchid-project.org/compounds/Al3Mo5.html) | -22 kJ/mol-atom |  | model |  | 0.223 (oqmd-1277798) | [4] Liu 2000; _cites Boer 1989_ | Table 5, p. 8, row 5; `ORC-CBFYDBTBRQ.96a41e` |  |
| Mo5Al3-D8m | [Al3Mo5](https://data.orchid-project.org/compounds/Al3Mo5.html) | -7.3 kJ/mol-atom |  | model |  | 0.223 (oqmd-1277798) | [4] Liu 2000 | Table 5, p. 8, row 6; `ORC-MLGRW4L3ME.abc837` |  |
| Mo5Al3–D8m | [Al3Mo5](https://data.orchid-project.org/compounds/Al3Mo5.html) | -23 kJ/mol-atom |  | model |  | 0.223 (oqmd-1277798) | [5] Guo 2012 | Table 3, p. 8, row 7; `ORC-KRFTD44W63.334d50` |  |
| Mo5Al3–D8m | [Al3Mo5](https://data.orchid-project.org/compounds/Al3Mo5.html) | -22 kJ/mol-atom |  | model |  | 0.223 (oqmd-1277798) | [5] Guo 2012; _cites Boer 1988_ | Table 3, p. 8, row 8; `ORC-YE3UC7GJLU.3052ae` |  |
| Mo5Al3–D8m | [Al3Mo5](https://data.orchid-project.org/compounds/Al3Mo5.html) | -7.3 kJ/mol-atom |  | model |  | 0.223 (oqmd-1277798) | [5] Guo 2012; _cites Liu 2000_ [doi](https://doi.org/10.1016/s0966-9795%2800%2900068-6) | Table 3, p. 8, row 9; `ORC-4KJDVHSCSI.653012` |  |
| MoAl2-C11b | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -20 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [4] Liu 2000; _cites Boer 1989_ | Table 5, p. 8, row 1; `ORC-JLZAOGJJBT.328ae1` |  |
| MoAl2-C11b | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -19 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [4] Liu 2000 | Table 5, p. 8, row 2; `ORC-WVLQ4WISQA.6f33a6` |  |
| MoAl2-C40 | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -21 kJ/mol-atom |  | model |  | -1.389 (oqmd-1797232) | [4] Liu 2000 | Table 5, p. 8, row 4; `ORC-UESQZ4UUIP.b53865` |  |
| MoAl2-C40 | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -20 kJ/mol-atom |  | model |  | -1.389 (oqmd-1797232) | [4] Liu 2000; _cites Boer 1989_ | Table 5, p. 8, row 3; `ORC-HHJ4CHRPJJ.298207` |  |
| MoAl2–C11b | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -20 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [5] Guo 2012; _cites Boer 1988_ | Table 3, p. 8, row 2; `ORC-7JSBSYKZ6K.8949c0` |  |
| MoAl2–C11b | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -20 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [5] Guo 2012 | Table 3, p. 8, row 1; `ORC-ZCVIFQH6NU.a5f740` |  |
| MoAl2–C11b | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -19 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [5] Guo 2012; _cites Liu 2000_ [doi](https://doi.org/10.1016/s0966-9795%2800%2900068-6) | Table 3, p. 8, row 3; `ORC-SY7ODGRE2F.89fb87` |  |
| MoAl2–C40 | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -22.2 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [5] Guo 2012 | Table 3, p. 8, row 4; `ORC-GP75YYNOIG.471b9e` |  |
| MoAl2–C40 | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -21 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [5] Guo 2012; _cites Liu 2000_ [doi](https://doi.org/10.1016/s0966-9795%2800%2900068-6) | Table 3, p. 8, row 6; `ORC-PXZB4QXQFZ.024f01` |  |
| MoAl2–C40 | [Al2Mo](https://data.orchid-project.org/compounds/Al2Mo.html) | -20 kJ/mol-atom |  | model |  | -2.255 (oqmd-1609942) | [5] Guo 2012; _cites Boer 1988_ | Table 3, p. 8, row 5; `ORC-6NRRY7GPV3.3db754` |  |

## Other properties

### Phase transition (7)

Table: Phase transition, Al–Mo system

| Property | Value | T (K) | Phases / composition | Class | Source | Location | Quote |
|---|---:|---:|---|---|---|---|---|
| Phase transition | 1120 K | 1120 | other | experimental | [2] Du 2009; _cites Ya 1970_ | p. 10; `ORC-ME72ENZBLQ.7d8f27` | “The decomposition temperatures of s1, s2 and e\*(Al5Fe4) are 1120, 1350 and 1353 K, respectively, which are basically in agreement with the experimental temperatures 1120,\[32\] 1344-1368\[45\] and 1358-1368 K.\[45\]” |
| Phase transition | 1120 K | 1120 | other | model | [2] Du 2009 | p. 10; `ORC-ME72ENZBLQ.ed2e12` | “The decomposition temperatures of s1, s2 and e\*(Al5Fe4) are 1120, 1350 and 1353 K, respectively, which are basically in agreement with the experimental temperatures 1120,\[32\] 1344-1368\[45\] and 1358-1368 K.\[45\]” |
| Phase transition | 1350 K | 1350 | other | model | [2] Du 2009 | p. 10; `ORC-ME72ENZBLQ.aa87a5` | “The decomposition temperatures of s1, s2 and e\*(Al5Fe4) are 1120, 1350 and 1353 K, respectively, which are basically in agreement with the experimental temperatures 1120,\[32\] 1344-1368\[45\] and 1358-1368 K.\[45\]” |
| Phase transition | 1819 K | 1819 | congruent transformation | experimental | [3] Cupid 2010; _cites Eumann 2006_ [doi](https://doi.org/10.3139/146.101412) | p. 5; `ORC-RBXX3IWQUV` | “The value of b was assigned to fit the congruent melting of Al8Mo3 at 1819 K measured by Eumann et al. \[43\].” |
| Phase transition | 1821 K | 1821 | congruent transformation | model | [3] Cupid 2010 | p. 8; `ORC-QPARLX7QBN` | “The congruent melting of Al8Mo3 is calculated at 1821 K, which is in good agreement with the thermal analysis measurements of Schuster and Ipser \[41\] (1828 10 K) and Eumann et al. \[43\] (1819 5 K).” |
| Phase transition | 2023 K | 2023 | congruent transformation | model | [3] Cupid 2010 | p. 8; `ORC-ZRDKGIRDXH` | “The b phase melts congruently at 2023 K, which is in excellent agreement with the critical evaluation of Schuster \[42\].” |
| Phase transition | 2323 K | 2323 | congruent transformation | experimental | [3] Cupid 2010 | p. 2; `ORC-RSMOFFZ24G.54a901` | “Al3Mo was shown to form peritectically at 1403 K and Al2Mo was shown to melt congruently at z2323 K.” |

### Phase equilibrium (29)

Table: Phase equilibrium, Al–Mo system

| Property | Value | T (K) | Phases / composition | Class | Source | Location | Quote |
|---|---:|---:|---|---|---|---|---|
| Phase composition |  | 673.15 | (Al); _(Al): Al 0.99972, Mo 2.800e-4_ | experimental | [1] Ltd. 1997; _cites ref. 60Vig_ | Table 2, p. 2, row 29; `ORC-PIWUIXUR5R` |  |
| Phase composition |  | 723.15 | (Al); _(Al): Al 0.99961, Mo 3.900e-4_ | experimental | [1] Ltd. 1997; _cites ref. 60Vig_ | Table 2, p. 2, row 28; `ORC-OQPMIA5A6E` |  |
| Phase composition |  | 773.15 | (Al); _(Al): Al 0.99955, Mo 4.500e-4_ | experimental | [1] Ltd. 1997; _cites ref. 60Vig_ | Table 2, p. 2, row 27; `ORC-MHGHPEGCFY` |  |
| Phase composition |  | 823.15 | (Al); _(Al): Al 0.99946, Mo 5.400e-4_ | experimental | [1] Ltd. 1997; _cites ref. 60Vig_ | Table 2, p. 2, row 26; `ORC-DKCKCBDRXJ` |  |
| Phase composition |  | 833.15 | (Al); _(Al): Al 0.99996, Mo 4.000e-5_ | experimental | [1] Ltd. 1997; _cites ref. 33Roe_ | Table 2, p. 2, row 23; `ORC-VBKTZIHJJE` |  |
| Phase composition |  | 913.15 | (Al); _(Al): Al 0.99938, Mo 6.200e-4_ | experimental | [1] Ltd. 1997; _cites ref. 60Vig_ | Table 2, p. 2, row 25; `ORC-6I34MRNWLY` |  |
| Phase composition |  | 933.15 | (Al); _(Al): Al 0.9994, Mo 6.000e-4_ | experimental | [1] Ltd. 1997; _cites L 1951_ | Table 2, p. 2, row 24; `ORC-4WOF3ZLYJT` |  |
| Phase composition |  | 938.15 | Liquid + L; _Liquid: Al 0.99968, Mo 3.200e-4; L: Al 0.99968, Mo 3.200e-4_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 22; `ORC-HMFMYOFZHV` |  |
| Phase composition |  | 958.15 | Liquid + L; _Liquid: Al 0.99952, Mo 4.800e-4; L: Al 0.99952, Mo 4.800e-4_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 21; `ORC-FYQU6YEC4U` |  |
| Phase composition |  | 973.15 | Liquid + L; _Liquid: Al 0.99939, Mo 6.100e-4; L: Al 0.99939, Mo 6.100e-4_ | experimental | [1] Ltd. 1997; _cites ref. 76Yer_ | Table 2, p. 2, row 11; `ORC-RYCQAJJGQ7` |  |
| Phase composition |  | 974.15 | Liquid + L; _Liquid: Al 0.9994, Mo 6.000e-4; L: Al 0.9994, Mo 6.000e-4_ | experimental | [1] Ltd. 1997; _cites ref. 40Yam_ | Table 2, p. 2, row 7; `ORC-UYICG6A2A5` |  |
| Phase composition |  | 978.15 | Liquid + L; _Liquid: Al 0.9991, Mo 9.000e-4; L: Al 0.9991, Mo 9.000e-4_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 20; `ORC-EPL4KZX6HB` |  |
| Phase composition |  | 988.15 | Liquid + L; _Liquid: Al 0.99907, Mo 9.300e-4; L: Al 0.99907, Mo 9.300e-4_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 19; `ORC-4PZ6OVAAEM` |  |
| Phase composition |  | 1013.15 | Liquid + L; _Liquid: Al 0.99907, Mo 9.300e-4; L: Al 0.99907, Mo 9.300e-4_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 18; `ORC-TKTDWROHEJ` |  |
| Phase composition |  | 1022.15 | Liquid + L; _Liquid: Al 0.9988, Mo 0.0012; L: Al 0.9988, Mo 0.0012_ | experimental | [1] Ltd. 1997; _cites ref. 40Yam_ | Table 2, p. 2, row 6; `ORC-GAGGTN2KQN` |  |
| Phase composition |  | 1023.15 | Liquid + L; _Liquid: Al 0.99876, Mo 0.00124; L: Al 0.99876, Mo 0.00124_ | experimental | [1] Ltd. 1997; _cites ref. 76Yer_ | Table 2, p. 2, row 10; `ORC-OOM4KELGUN` |  |
| Phase composition |  | 1063.15 | Liquid + L; _Liquid: Al 0.99788, Mo 0.00212; L: Al 0.99788, Mo 0.00212_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 17; `ORC-Z4DNSMSZQL` |  |
| Phase composition |  | 1073.15 | Liquid + L; _Liquid: Al 0.99799, Mo 0.00201; L: Al 0.99799, Mo 0.00201_ | experimental | [1] Ltd. 1997; _cites ref. 76Yer_ | Table 2, p. 2, row 9; `ORC-WAQKNLBN5W` |  |
| Phase composition |  | 1074.15 | Liquid + L; _Liquid: Al 0.998, Mo 0.002; L: Al 0.998, Mo 0.002_ | experimental | [1] Ltd. 1997; _cites ref. 40Yam_ | Table 2, p. 2, row 5; `ORC-VVZGFNYCK4` |  |
| Phase composition |  | 1103.15 | Liquid + L; _Liquid: Al 0.99725, Mo 0.00275; L: Al 0.99725, Mo 0.00275_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 16; `ORC-3T7CZRYEMZ` |  |
| Phase composition |  | 1123.15 | Liquid + L; _Liquid: Al 0.99677, Mo 0.00323; L: Al 0.99677, Mo 0.00323_ | experimental | [1] Ltd. 1997; _cites ref. 76Yer_ | Table 2, p. 2, row 8; `ORC-T6OWDPSDAP` |  |
| Phase composition |  | 1125.15 | Liquid + L; _Liquid: Al 0.9965, Mo 0.0035; L: Al 0.9965, Mo 0.0035_ | experimental | [1] Ltd. 1997; _cites ref. 40Yam_ | Table 2, p. 2, row 4; `ORC-SSG4J2APC7` |  |
| Phase composition |  | 1169.15 | Liquid + L; _Liquid: Al 0.9945, Mo 0.0055; L: Al 0.9945, Mo 0.0055_ | experimental | [1] Ltd. 1997; _cites ref. 40Yam_ | Table 2, p. 2, row 3; `ORC-KWJZQGWQQ4` |  |
| Phase composition |  | 1173.15 | Liquid + L; _Liquid: Al 0.99453, Mo 0.00547; L: Al 0.99453, Mo 0.00547_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 15; `ORC-RQEBWCZU5Q` |  |
| Phase composition |  | 1178.15 | Liquid + L; _Liquid: Al 0.99412, Mo 0.00588; L: Al 0.99412, Mo 0.00588_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 14; `ORC-OG6ATETTQQ` |  |
| Phase composition |  | 1208.15 | Liquid + L; _Liquid: Al 0.9927, Mo 0.0073; L: Al 0.9927, Mo 0.0073_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 13; `ORC-R4PQO6JDS3` |  |
| Phase composition |  | 1218.15 | Liquid + L; _Liquid: Al 0.9931, Mo 0.0069; L: Al 0.9931, Mo 0.0069_ | experimental | [1] Ltd. 1997; _cites ref. 40Yam_ | Table 2, p. 2, row 2; `ORC-J2TQ5WMHEP` |  |
| Phase composition |  | 1273.15 | Liquid + L; _Liquid: Al 0.98785, Mo 0.01215; L: Al 0.98785, Mo 0.01215_ | experimental | [1] Ltd. 1997; _cites ref. 80Mal_ | Table 2, p. 2, row 12; `ORC-OU334H63KH` |  |
| Phase composition |  | 1273.15 | Liquid + L; _Liquid: Al 0.9906, Mo 0.0094; L: Al 0.9906, Mo 0.0094_ | experimental | [1] Ltd. 1997; _cites ref. 40Yam_ | Table 2, p. 2, row 1; `ORC-TRPZSBMCT2` |  |

### Mixing / partial (8)

Table: Mixing / partial, Al–Mo system

| Property | Value | T (K) | Phases / composition | Class | Source | Location | Quote |
|---|---:|---:|---|---|---|---|---|
| Enthalpy of mixing; _printed: ΔHexp_ | -18.05 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.82, Mo 0.18_ | experimental | [1] Ltd. 1997; _cites Sudsatsova 1985_ | Table 7, p. 6, row 7; `ORC-DGGNOBWTGG` |  |
| Enthalpy of mixing; _printed: ΔHcalc_ | -5.46 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.95, Mo 0.05_ | model | [1] Ltd. 1997 | Table 7, p. 6, row 2; `ORC-G7MXQJQTC3` |  |
| Enthalpy of mixing; _printed: ΔHexp_ | -15.02 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.85, Mo 0.15_ | experimental | [1] Ltd. 1997; _cites Sudsatsova 1985_ | Table 7, p. 6, row 5; `ORC-GBEWWNVM6Y` |  |
| Enthalpy of mixing; _printed: ΔHcalc_ | -10.33 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.9, Mo 0.1_ | model | [1] Ltd. 1997 | Table 7, p. 6, row 4; `ORC-I6D563T5SA` |  |
| Enthalpy of mixing; _printed: ΔHexp_ | -5.05 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.95, Mo 0.05_ | experimental | [1] Ltd. 1997; _cites Sudsatsova 1985_ | Table 7, p. 6, row 1; `ORC-QENWJMGEMD` |  |
| Enthalpy of mixing; _printed: ΔHexp_ | -10.04 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.9, Mo 0.1_ | experimental | [1] Ltd. 1997; _cites Sudsatsova 1985_ | Table 7, p. 6, row 3; `ORC-Y2YO7PC4CT` |  |
| Enthalpy of mixing; _printed: ΔHcalc_ | -16.88 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.82, Mo 0.18_ | model | [1] Ltd. 1997 | Table 7, p. 6, row 8; `ORC-YBA5AXUPR4` |  |
| Enthalpy of mixing; _printed: ΔHcalc_ | -14.61 kJ/mol (basis unstated) |  | Liquid; _alloy: Al 0.85, Mo 0.15_ | model | [1] Ltd. 1997 | Table 7, p. 6, row 6; `ORC-ZIIARAO7LH` |  |

### Crystal structure (36)

Table: Crystal structure, Al–Mo system

| Property | Value | T (K) | Phases / composition | Class | Source | Location | Quote |
|---|---:|---:|---|---|---|---|---|
| Lattice a | 7.5815 Å | 298.15 | Al12Mo; _Al12Mo: Al 0.9223, Mo 0.0777_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 2; `ORC-BKQWI6IF2T` |  |
| Lattice a | 7.5877 Å | 298.15 | Al12Mo; _alloy: Mo 0.076923_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 12; `ORC-R6L355IDRN` |  |
| Lattice a | 4.945 Å ± 0.001 | 298.15 | Al3+xMo1-x; _alloy: Mo 0.25_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 20; `ORC-H2MUDWTO7O` |  |
| Lattice a | 16.396 Å ± 0.001 | 298.15 | Al3Mo; _alloy: Mo 0.25_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 21; `ORC-DZLZGYDP7D.72e99f` |  |
| Lattice a | 5.255 Å | 298.15 | Al4Mo; _Al4Mo: Al 0.8, Mo 0.2_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 4; `ORC-HWWKMT3IIY.9107d0` |  |
| Lattice a | 5.26 Å ± 0.002 | 298.15 | Al4Mo; _alloy: Mo 0.2_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 19; `ORC-JZINBCHMOA.2dcece` |  |
| Lattice a | 4.89 Å | 298.15 | Al5Mo; _Al5Mo: Al 0.833, Mo 0.167_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 3; `ORC-GWPLYECOII.2c71a0` |  |
| Lattice a | 4.912 Å ± 0.002 | 298.15 | Al5Mo(h); _alloy: Mo 0.166667_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 14; `ORC-VARHOUE6QX.84bf45` |  |
| Lattice a | 4.933 Å ± 0.001 | 298.15 | Al5Mo(m); _alloy: Mo 0.166667_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 15; `ORC-OIYPV4REBS.3e3cee` |  |
| Lattice a | 4.951 Å ± 0.001 | 298.15 | Al5Mo(r); _alloy: Mo 0.166667_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 16; `ORC-4GAXHW7FJN.3a6785` |  |
| Lattice a | 5.12 Å | 298.15 | Al7Mo(a); _alloy: Mo 0.125_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 13; `ORC-2CMHCNKVSP.157c28` |  |
| Lattice a | 9.207 Å ± 0.003 | 298.15 | Al8Mo3; _alloy: Mo 0.272727_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 22; `ORC-U7GPZHRYFT.ff6338` |  |
| Lattice a | 9.208 Å | 298.15 | Al8Mo3; _Al8Mo3: Al 0.687, Mo 0.313_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 5; `ORC-YPC53GCDVQ.ce0c5d` |  |
| Lattice a | 3.089 Å | 298.15 | AlMo; _AlMo: Al 0.46, Mo 0.54_ | unspecified | [1] Ltd. 1997; _cites ref. 71Rex_ | Table 5, p. 5, row 13; `ORC-5RHKM5I376` |  |
| Lattice a | 3.098 Å | 298.15 | AlMo; _AlMo: Al 0.52, Mo 0.48_ | unspecified | [1] Ltd. 1997; _cites ref. 71Rex_ | Table 5, p. 5, row 12; `ORC-Y52OTI43BA` |  |
| Lattice a | 4.95 Å | 298.15 | AlMo3; _AlMo3: Al 0.75, Mo 0.25; Al3Mo: Al 0.75, Mo 0.25_ | experimental | [1] Ltd. 1997; _cites "Beta Wolfram Structure of Compounds Between Transition Elements and AI 1958_ | Table 5, p. 5, row 11; `ORC-KNLNF5PS5V` |  |
| Lattice b | 3.594 Å ± 0.001 | 298.15 | Al3Mo; _alloy: Mo 0.25_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 21; `ORC-DZLZGYDP7D.04a37d` |  |
| Lattice b | 17.768 Å | 298.15 | Al4Mo; _Al4Mo: Al 0.8, Mo 0.2_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 4; `ORC-HWWKMT3IIY.40533d` |  |
| Lattice b | 17.785 Å ± 0.003 | 298.15 | Al4Mo; _alloy: Mo 0.2_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 19; `ORC-JZINBCHMOA.f99375` |  |
| Lattice b | 13 Å | 298.15 | Al7Mo(a); _alloy: Mo 0.125_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 13; `ORC-2CMHCNKVSP.97288a` |  |
| Lattice b | 3.641 Å ± 0.001 | 298.15 | Al8Mo3; _alloy: Mo 0.272727_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 22; `ORC-U7GPZHRYFT.b327ff` |  |
| Lattice b | 3.6378 Å | 298.15 | Al8Mo3; _Al8Mo3: Al 0.687, Mo 0.313_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 5; `ORC-YPC53GCDVQ.380719` |  |
| Lattice c | 8.386 Å ± 0.004 | 298.15 | Al3Mo; _alloy: Mo 0.25_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 21; `ORC-DZLZGYDP7D.264292` |  |
| Lattice c | 5.255 Å | 298.15 | Al4Mo; _Al4Mo: Al 0.8, Mo 0.2_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 4; `ORC-HWWKMT3IIY.923a5c` |  |
| Lattice c | 5.226 Å ± 0.001 | 298.15 | Al4Mo; _alloy: Mo 0.2_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 19; `ORC-JZINBCHMOA.93a7ee` |  |
| Lattice c | 8.8 Å | 298.15 | Al5Mo; _Al5Mo: Al 0.833, Mo 0.167_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 3; `ORC-GWPLYECOII.27cf2d` |  |
| Lattice c | 8.86 Å ± 0.004 | 298.15 | Al5Mo(h); _alloy: Mo 0.166667_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 14; `ORC-VARHOUE6QX.73c20c` |  |
| Lattice c | 43.98 Å ± 0.09 | 298.15 | Al5Mo(m); _alloy: Mo 0.166667_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 15; `ORC-OIYPV4REBS.131c8a` |  |
| Lattice c | 26.23 Å ± 0.01 | 298.15 | Al5Mo(r); _alloy: Mo 0.166667_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 16; `ORC-4GAXHW7FJN.3c982e` |  |
| Lattice c | 13.5 Å | 298.15 | Al7Mo(a); _alloy: Mo 0.125_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 13; `ORC-2CMHCNKVSP.de3fe3` |  |
| Lattice c | 10.06 Å ± 0.05 | 298.15 | Al8Mo3; _alloy: Mo 0.272727_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 22; `ORC-U7GPZHRYFT.1b9aef` |  |
| Lattice c | 10.065 Å | 298.15 | Al8Mo3; _Al8Mo3: Al 0.687, Mo 0.313_ | unspecified | [1] Ltd. 1997 | Table 5, p. 5, row 5; `ORC-YPC53GCDVQ.5720d9` |  |
| lattice beta | 95 ° | 298.15 | Al7Mo(a); _alloy: Mo 0.125_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 13; `ORC-2CMHCNKVSP.fb958a` |  |
| lattice unlabelled value | 101.88 not_printed ± 0.07 | 298.15 | Al3Mo; _alloy: Mo 0.25_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 21; `ORC-DZLZGYDP7D.1afbc0` |  |
| lattice unlabelled value | 100.15 not_printed ± 0.05 | 298.15 | Al4Mo; _alloy: Mo 0.2_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 19; `ORC-JZINBCHMOA.249db6` |  |
| lattice unlabelled value | 100.78 not_printed ± 0.09 | 298.15 | Al8Mo3; _alloy: Mo 0.272727_ | unspecified | [1] Ltd. 1997; _cites ref. 91Sch_ | Table A1, p. 8, row 22; `ORC-U7GPZHRYFT.5bb5d2` |  |

## Sources

Reporting papers the values were read from (a value cited from another work names that work in its row).

1. Thermotech Ltd., N. Saunders, The Al-Mo system (aluminum-molybdenum), JPE 18, 370-378 (1997). [doi:10.1007/s11669-997-0063-1](https://doi.org/10.1007/s11669-997-0063-1)
2. Zhenmin Du, Cuiping Guo, Changrong Li, Weijing Zhang, Thermodynamic Description of the Al-Mo and Al-Fe-Mo Systems, J. Phase Equilib. Diffus. 30, 487-501 (2009). [doi:10.1007/s11669-009-9564-4](https://doi.org/10.1007/s11669-009-9564-4)
3. Damian M. Cupid, Olga Fabrichnaya, Fereshteh Ebrahimi, Hans J. Seifert, Thermodynamic assessment of the Al–Mo system and of the Ti–Al–Mo System from 0 to 20at.% Ti, Intermetallics 18, 1185-1196 (2010). [doi:10.1016/j.intermet.2010.03.010](https://doi.org/10.1016/j.intermet.2010.03.010)
4. Y Liu, G Shao, P Tsakiropoulos, Thermodynamic reassessment of the Mo–Si and Al–Mo–Si systems, Intermetallics 8, 953-962 (2000). [doi:10.1016/s0966-9795(00)00068-6](https://doi.org/10.1016/s0966-9795%2800%2900068-6)
5. Cuiping Guo, Changrong Li, Patrick J. Masset, Zhenmin Du, A thermodynamic description of the Al–Mo–Si system, Calphad 36, 100-109 (2012). [doi:10.1016/j.calphad.2011.12.003](https://doi.org/10.1016/j.calphad.2011.12.003)

## Please cite

- R. Arróyave, J. Saal, D. Shin, ORCHID-Values: thermodynamic and phase-equilibrium values read from the literature (version 2026.10; Version 1, machine-extracted), Zenodo (2026). https://doi.org/10.5281/zenodo.23735569
- R. Arróyave, J. Saal, D. Shin, ORCHID-Diagrams: calculated binary phase diagrams (version 2026.10), Zenodo (2026). https://doi.org/10.5281/zenodo.23735859
- R. Arróyave, J. Saal, D. Shin, ORCHID-Hulls: binary convex hulls (Materials Project, OQMD, assessed CALPHAD) (version 2026.10), Zenodo (2026). https://doi.org/10.5281/zenodo.23735891
- R. Arróyave, J. Saal, D. Shin, ORCHID data: umbrella record of the ORCHID datasets (version 2026.10; Version 1, machine-extracted), Zenodo (2026). https://doi.org/10.5281/zenodo.23736065

Also cite the original source of every value you use (paper_citation / paper_doi, and cited_dois for values the paper cites from earlier work); B. Hallstedt, The SGTE collection of binary datasets, Calphad 89 (2025) 102833, https://doi.org/10.1016/j.calphad.2025.102833 (CC BY 4.0), and the original assessment named in each file; A. Jain et al., The Materials Project: A materials genome approach to accelerating materials innovation, APL Materials 1 (2013) 011002, https://doi.org/10.1063/1.4812323 (CC BY 4.0); J. E. Saal et al., JOM 65 (2013) 1501, https://doi.org/10.1007/s11837-013-0755-4 and S. Kirklin et al., npj Comput. Mater. 1 (2015) 15010, https://doi.org/10.1038/npjcompumats.2015.10 (CC BY 4.0).

Version 1, machine-extracted: values were read by language-model readers constrained to quote their source and checked automatically, and the release was then audited on the printed pages by adversarial audits, an independent second review of fit-facing records and a preliminary human review of a frozen sample. Flags such as accepted and ESPEI-ready record screening results, not certification; known issues are listed in the release notes.

```bibtex
@misc{orchid_literature_2026,
  author    = {Arr{\'o}yave, Raymundo and Saal, James and Shin, Dongwon},
  title     = {{ORCHID-Values: thermodynamic and phase-equilibrium values read from the literature}},
  version   = {2026.10},
  publisher = {Zenodo},
  year      = {2026},
  doi       = {10.5281/zenodo.23735569},
  url       = {https://doi.org/10.5281/zenodo.23735569},
  note      = {Version 1, machine-extracted}
}

@misc{orchid_phase_diagrams_2026,
  author    = {Arr{\'o}yave, Raymundo and Saal, James and Shin, Dongwon},
  title     = {{ORCHID-Diagrams: calculated binary phase diagrams}},
  version   = {2026.10},
  publisher = {Zenodo},
  year      = {2026},
  doi       = {10.5281/zenodo.23735859},
  url       = {https://doi.org/10.5281/zenodo.23735859}
}

@misc{orchid_hulls_2026,
  author    = {Arr{\'o}yave, Raymundo and Saal, James and Shin, Dongwon},
  title     = {{ORCHID-Hulls: binary convex hulls (Materials Project, OQMD, assessed CALPHAD)}},
  version   = {2026.10},
  publisher = {Zenodo},
  year      = {2026},
  doi       = {10.5281/zenodo.23735891},
  url       = {https://doi.org/10.5281/zenodo.23735891}
}

@misc{orchid_data_2026,
  author    = {Arr{\'o}yave, Raymundo and Saal, James and Shin, Dongwon},
  title     = {{ORCHID data: umbrella record of the ORCHID datasets}},
  version   = {2026.10},
  publisher = {Zenodo},
  year      = {2026},
  doi       = {10.5281/zenodo.23736065},
  url       = {https://doi.org/10.5281/zenodo.23736065},
  note      = {Version 1, machine-extracted}
}
```

---

Derived data CC BY 4.0 ([licence](https://creativecommons.org/licenses/by/4.0/)): cite ORCHID ([CITATION.cff](https://data.orchid-project.org/CITATION.cff)) and the original sources. Quotes are short excerpts kept so that each value can be checked; they remain under the publishers' copyright and are not relicensed. Source papers, page images and full text are not redistributed. Field reference: [SCHEMA.md](https://data.orchid-project.org/literature/SCHEMA.md). Machine-readable guide: [llms.txt](https://data.orchid-project.org/llms.txt). Found an error? The report link of a value (Markdown: its id, ORC-..., in the Location column) opens a pre-filled GitHub issue, https://github.com/orchid-calphad/orchid-data/issues/new?template=report-value-error.yml&record_id=\<id>, carrying only the record id, source and value; [how to contribute](https://orchid-project.org/contribute/).