Bi–Ca–Cu–O–Sr system
30 accepted literature values from 1 paper(s) (experimental 15, unspecified 15); 0 calculated phase diagram(s).
Data: JSON · CSV · interactive explorer · papers (bibliography) · Markdown
| Evidence class | Values |
|---|---|
| experimental | 15 |
| unspecified | 15 |
| Property group | Values |
|---|---|
| phase transition | 30 |
Other properties
Phase transition (30)
| Property | Value | T (K) | Phases / composition | Class | Source | Location | Quote |
|---|---|---|---|---|---|---|---|
| Phase transition | 1133 K | 1133 | CaO min, exp., 0.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 21 report | |
| Phase transition | 1147 K | 1147 | 01x1 max, calc., 0.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 10 report | |
| Phase transition | 1148 K | 1148 | 01x1 max, exp., 0.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 7 report | |
| Phase transition | 1159 K | 1159 | 02x1 max, exp., 0.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 16 report | |
| Phase transition | 1173 K | 1173 | 02x1 min, calc., 0.21 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 14 report | |
| Phase transition | 1173 K | 1173 | 02x1 min, exp., 0.21 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 12 report | |
| Phase transition | 1183 K | 1183 | 23x0 max, exp., 0.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 29 report | |
| Phase transition | 1189 K | 1189 | 91150 max, calc., 0.21 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 28 report | |
| Phase transition | 1193 K | 1193 | 91150 max, exp., 0.21 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 26 report | |
| Phase transition | 1195 K | 1195 | 23x0 max, calc., 0.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 30 report | |
| Phase transition | 1198 K | 1198 | CaO min, calc., 0.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 24 report | |
| Phase transition | 1203 K | 1203 | 01x1 max, exp., 0.21 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 6 report | |
| Phase transition | 1204 K | 1204 | 01x1 max, calc., 0.21 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 9 report | |
| Phase transition | 1205 K | 1205 | 02x1 min, calc., 1.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 13 report | |
| Phase transition | 1210 K | 1210 | 014x24 max, calc., 1.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 2 report | |
| Phase transition | 1210 K | 1210 | 01x1 min, calc., 1.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 4 report | |
| Phase transition | 1210 K | 1210 | CaO min, exp., 0.21 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 20 report | |
| Phase transition | 1215 K | 1215 | 02x1 min, exp., 1.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 11 report | |
| Phase transition | 1216 K | 1216 | 014x24 max, exp., 1.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 1 report | |
| Phase transition | 1216 K | 1216 | 01x1 min, exp., 1.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 3 report | |
| Phase transition | 1219 K | 1219 | 91150 max, calc., 1.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 27 report | |
| Phase transition | 1223 K | 1223 | 02x1 max, exp., 0.21 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 15 report | |
| Phase transition | 1232 K | 1232 | 01x1 max, calc., 1.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 8 report | |
| Phase transition | 1233 K | 1233 | 01x1 max, exp., 1.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 5 report | |
| Phase transition | 1236 K | 1236 | 91150 max, exp., 1.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 25 report | |
| Phase transition | 1239 K | 1239 | CaO min, exp., 1.01 bar O2 | experimental | [1] Hallstedt 2003 cites Margulies 1996 doi | Table 8, p. 12, row 19 report | |
| Phase transition | 1244 K | 1244 | 02x1 max, calc., 0.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 18 report | |
| Phase transition | 1263 K | 1263 | CaO min, calc., 0.21 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 23 report | |
| Phase transition | 1295 K | 1295 | CaO min, calc., 1.01 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 22 report | |
| Phase transition | 1299 K | 1299 | 02x1 max, calc., 0.21 bar O2 | unspecified | [1] Hallstedt 2003 | Table 8, p. 12, row 17 report |
Sources
Reporting papers the values were read from (a value cited from another work names that work in its row).
- Bengt Hallstedt, Ludwig J. Gauckler, Revision of the thermodynamic descriptions of the Cu–O, Ag–O, Ag–Cu–O, Bi–Sr–O, Bi–Ca–O, Bi–Cu–O, Sr–Cu–O, Ca–Cu–O and Sr–Ca–Cu–O systems, Calphad 27, 177-191 (2003). doi:10.1016/s0364-5916(03)00050-6