Sn–V system
9 accepted literature values from 1 paper(s) (experimental 2, unspecified 7); 2 calculated phase diagram(s).
Data: JSON · CSV · interactive explorer · interactive phase diagram · phases (9) · papers (bibliography) · Markdown
| Evidence class | Values |
|---|---|
| experimental | 2 |
| unspecified | 7 |
| Property group | Values |
|---|---|
| phase equilibrium | 9 |
Calculated phase diagrams
Binary phase diagrams calculated with pycalphad 0.11.2 from the SGTE binary collection (Hallstedt 2025, CC BY 4.0). Evidence class: model.
| TDB file | Assessment | SHA-256 | Links |
|---|---|---|---|
| SnV-02Stu-LB.tdb | T. Studnitzky, B. Onderka, R. Schmid-Fetzer, Z. Metallkd., 93, 48-57(2002). doi:10.3139/ijmr-2002-0009 | 34ad8b6e7351ecab2b1c5915a9b47acaf8bc19937978f699ccdbf1609030f13b | viewer · TDB · JSON |
| SnV-08Che.tdb | C.-C. Chen, W. Gierlotka, S.-W. Chen, J. Electron. Mater., 37, 1727-33(2008). doi:10.1007/s11664-008-0530-4 | 8c98bca6360bcce78406b38a2648cf5875edff285a0979cd868587c45fdda28b | viewer · TDB · JSON |
| TDB file | T (K) | Phases at the invariant |
|---|---|---|
| SnV-02Stu-LB.tdb | 1871.31 | LIQUID (x(V) 0.62387) + SNV3_A15 (x(V) 0.795) + BCC_A2 (x(V) 0.84492) |
| SnV-02Stu-LB.tdb | 1871.31 | LIQUID (x(V) 0.62399) + SNV3_A15 (x(V) 0.795) + BCC_A2 (x(V) 0.84494) |
| SnV-02Stu-LB.tdb | 1773.39 | LIQUID#2 (x(V) 0.15636) + LIQUID (x(V) 0.41662) + SNV3_A15 (x(V) 0.795) |
| SnV-02Stu-LB.tdb | 1032.2 | LIQUID (x(V) 0.00165) + SN3V2_CB (x(V) 0.4) + SNV3_A15 (x(V) 0.795) |
| SnV-02Stu-LB.tdb | 1032.2 | LIQUID (x(V) 0.00165) + SN3V2_CB (x(V) 0.4) + SNV3_A15 (x(V) 0.795) |
| SnV-02Stu-LB.tdb | 505.08 | BCT_A5 (x(V) 0) + LIQUID (x(V) 0) + SN3V2_CB (x(V) 0.4) |
| SnV-08Che.tdb | 1863.82 | LIQUID (x(V) 0.6238) + SNV3_A15 (x(V) 0.78) + BCC_A2 (x(V) 0.84194) |
| SnV-08Che.tdb | 1863.82 | LIQUID (x(V) 0.62401) + SNV3_A15 (x(V) 0.78) + BCC_A2 (x(V) 0.842) |
| SnV-08Che.tdb | 1775.19 | LIQUID#2 (x(V) 0.15744) + LIQUID (x(V) 0.41561) + SNV3_A15 (x(V) 0.78) |
| SnV-08Che.tdb | 1027.42 | LIQUID (x(V) 0.00146) + SN2V_CB (x(V) 0.34) + SNV3_A15 (x(V) 0.78) |
| SnV-08Che.tdb | 1027.42 | LIQUID (x(V) 0.00145) + SN2V_CB (x(V) 0.34) + SNV3_A15 (x(V) 0.78) |
| SnV-08Che.tdb | 505.08 | BCT_A5 (x(V) 0) + LIQUID (x(V) 0) + SN2V_CB (x(V) 0.34) |
Convex hulls: Materials Project DFT hull · OQMD DFT hull · CALPHAD hull SnV-02Stu-LB
Other properties
Phase equilibrium (9)
| Property | Value | T (K) | Phases / composition | Class | Source | Location | Quote |
|---|---|---|---|---|---|---|---|
| Phase assemblage | 523.15 | liquid + V2Sn3 alloy: V 0.2 | experimental | [1] Chen 2008 | p. 2 report | Figure 1 shows a BEI micrograph of alloy #1 (Sn-20.0at.%V) annealed at 250°C for 6 months. Two different phase regions are observed. The composition of the bright phase is Sn-0.1at.%V while that of the dark phase is Sn-33.7at.%V. | |
| Phase assemblage | 873.15 | V3Sn + V alloy: V 0.85 | experimental | [1] Chen 2008 | p. 3 report | Figure 5 shows the BEI micrograph of alloy #6 (Sn-85.0at.%V) annealed at 600°C for 9 months. Two phases are observed. The composition of the bright phase is Sn-78.0at.%V while that of the dark phase is Sn-87.7at.%V; these are the V3Sn phase and V phase, respectively. | |
| Phase composition | 523.15 | Liquid + VSn2(V2Sn3) Liquid: Sn 1, V 0; VSn2(V2Sn3): Sn 0.659, V 0.341 | unspecified | [1] Chen 2008 | Table I, p. 2, row 2 report | ||
| Phase composition | 523.15 | Liquid + VSn2(V2Sn3) Liquid: Sn 0.999, V 0.001; VSn2(V2Sn3): Sn 0.663, V 0.337 | unspecified | [1] Chen 2008 | Table I, p. 2, row 1 report | ||
| Phase composition | 523.15 | Liquid + VSn2(V2Sn3) Liquid: Sn 1, V 0; VSn2(V2Sn3): Sn 0.661, V 0.339 | unspecified | [1] Chen 2008 | Table I, p. 2, row 3 report | ||
| Phase composition | 523.15 | V3Sn + V V3Sn: Sn 0.219, V 0.781; V: Sn 0.121, V 0.879 | unspecified | [1] Chen 2008 | Table I, p. 2, row 7 report | ||
| Phase composition | 523.15 | VSn2(V2Sn3) + V3Sn VSn2(V2Sn3): Sn 0.659, V 0.341; V3Sn: Sn 0.218, V 0.782 | unspecified | [1] Chen 2008 | Table I, p. 2, row 5 report | ||
| Phase composition | 873.15 | V3Sn + V V3Sn: Sn 0.22, V 0.78; V: Sn 0.123, V 0.877 | unspecified | [1] Chen 2008 | Table I, p. 2, row 6 report | ||
| Phase composition | 873.15 | VSn2(V2Sn3) + V3Sn VSn2(V2Sn3): Sn 0.658, V 0.342; V3Sn: Sn 0.22, V 0.78 | unspecified | [1] Chen 2008 | Table I, p. 2, row 4 report |
Sources
Reporting papers the values were read from (a value cited from another work names that work in its row).
- Chih-Chi Chen, Wojcieh Gierlotka, Sinn-Wen Chen, Phase Equilibria of the Sn-V System and Interfacial Reactions in Sn/V Couples, Journal of Elec Materi 37, 1727-1733 (2008). doi:10.1007/s11664-008-0530-4